Science – Society – Technology
From: Casing failure identification of long-abandoned geothermal wells in Field Dieng, Indonesia
Well | Production casing data | Burst (MPa) | Collapse (MPa) | Tension (kN) | ||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|
Casing grade/pounder | Casing depth (m TVD/MD) | Resultant (design factor) | Burst ratinga | Evaluation | Resultant (design factor) | Collapse ratinga | Evaluation | Resultant (design factor) | Tension ratinga | Evaluation | ||
HCE9B | 339.7 mm K-55 101.2 kg/m | Top | 0 | 38.7 | 23.8 | Failed | 0 | 13.4 | Accepted | 3073 | 4755 | Accepted |
Bottom | 1519/1613 | 23.8 | 18.1 | Failed | 45 | 10.2 | Failed | 0 | 3614 | Accepted | ||
HCE28B | 339.7 mm K-55 101.2 kg/m | Top | 0 | 40 | 23.8 | Failed | 0 | 13.4 | Accepted | 2930 | 4755 | Accepted |
Bottom | 1504/1538 | 25.7 | 16.7 | Failed | 40 | 9.4 | Failed | 0 | 3337 | Accepted | ||
Tieback 273.1Â mm L-80 82.3Â kg/m | Top | 0 | 40 | 44.5 | Accepted | 0 | 27.7 | Accepted | 2391 | 5676 | Accepted | |
Bottom | 1504/1538 | 25.7 | 31.2 | Accepted | 40 | 19.5 | Failed | 0 | 3983 | Accepted |